INTRODUCTION Magnesium
in Superalloys
Magnesium
is
temperature
and
ductility
is
of
magnesium
improves
the
or
melted.
VIM
desulphurizing
Additions metals
decrease
virgin
heat.
suggested
help
in
improve both
terms
it has 192 .
strength
high
from
of
standpoint
Further,
fatigue
to
important
in-service
importance. low cycle
is
particularly the
added,
of the
starts
Following
the or
are
additions
from
cycle
scrap.
When
from
property
view,
also
superalloys
open-die
where
been
the
rupture
suggested
that
Melting
A typical materials
of
primary
Vacuum Induction
nickel-based
This
point
forgeability,
pick-up
to
ductility.
manufacturing
elements 3 cast .
added
with
mechanism
the
metal
is
deoxidizing
aluminum
and
activity of
of globurizing
down, molten
additions
are
bath
of the
the
or
of
oxygen
during
the
revert
heat
of
oxygen-containing
the alumina
cases, clusters
Superalloys 1988 Edited by S. Reichman, D.N. Duhl, G. Maurer, S. Antolovich and C. Lund The Metallurgical Society, 1988
raw
contents
are
bath
correct
(AE)
both
virgin
stable,
Finally,
is
In
407
furnace
made.
earth
in
either
and
composition
alkaline
oxygen
removal
charging
pumping
and content
refractories. the
the
entirely
and when the
The increase the
with
reactive the
rare is
however .
is
earth
(RE)
the melting
of a
probably the
inclusions 4
melt
due to
AE or by
RE the
Calcium, desulphurizing
agents.
be reduced the
and
magnesium, from
crucible
-
Figure
desulphurizing
-
agent
the
is
sulphur
critical
can be predicted
are
for
that
also
content
The sulphide
10 ppm.
it
Hence,
metals
earth
1 shows that
150 ppm to
walls.
rare
can readily
products the
strong
deposit
correct
on
amount
of
each charge4.
+ on molt- down 0 at malt end 200*-*-
Fic
/-
*---f
5 IOO-
/ J
0
-
12345678 HEAT
Figure
1:
Reduction induction
Alexander4 controlled
by
controlling
steps the
activity
of magnesium
process
latter data
during
the
mass
are
However, additional
that
liquid
liquid
is
removal
transfer
of
for
nickel
required
and the of better
alloys
for
Vacuum Induction
lack
[S]
is
equal
more accurate
over
vacuum
magnesium from VIM melts is 5 suggest that the Fu et al
while
mass transfer
were forced, in
sulphu r content . period
in melt melting
suggests
No.
evaporation data
reaction.
to assume that
to the
Clearly,
content.
analysis
of
the
the
evaporation
Melting.
Vacuum Arc Remelting Fu et al5 superalloy the
investigated
during
electrode
by the
the analysis Electra
It of
found
magnesium is
of magnesiuim
that
was suggested
of the problem
magnesium
that
through
the
the
limited
evaporates
evaporation
melt
by lack
from a nickel-base
to
the
mainly
rate
is
surface.
of fundamental
from
limited However,
data.
Slag Remelting
Ichihashi
et al6 aluminum,
titanium, compositions. increase
They
VAR.
tip.
transport
the evaporation
the
They content
investigated and
the ability
magnesium
show that
in
increasing
of magnesium
in
the
408
the the ingot,
of the ESR process metal contents
using
to retain
different
slag
of CaO and MgO will
as seen in Figure
2.
They
also
suggest
following
that
titanium
or
aluminum
can
be
lost
to
the
slag
through
reactions: 3MgO + 2E
+ A1203 + 3 Mg
2MgO + -Ti 2 TiO 2+2Mg
r-----l 0: 0: a: .:
150
CaO>2Sm0 15rCa052 5~CaOrls caos5
.(CaF,-MgO)
MgO (molX)
Figure
2:
Simultaneously, alloy. is
these
It
Ichihasi6 the
on
also
slag
is
argon.
reactions
may be noted
dependent
'n the ESR slag b.
Effect of MgO content in produced ESR ingots
a
that
proper
delicate
found
that
protected
Generally,
would
control
balance magnesium
from the
increase
air
the magnesium of
the reactive
between can not
oxidation
conclusions
of
on Mg content
slag
et
al.
has
recently
metal
chemistry. unless
atmosphere, 7
agree
the
content
in the metal
by an inert Chen
in
element
and
be retained
content
with
such
as
those
of
Ichihashi'. Electron
Beam Melting
The
Electron
alternative form
for
of
in
able. is
the
of
important
if
Mitchell' from
Refining
the
charge
superalloys
knowledge
of
desired
alloy
during
However,
makes evaporation evaporation
compositions
and Herbertsonl'
offers
the VAR process,
material. the
of
EBCHR refining.
the
as
another
applied
in the
more flexibility since
of
as
the heat
large
alloying
parameters
area
source
to volume
elements
unavoid-
alloying
elements
are to be produced.
have discussed
409
emerged usually
The process,
(EBCHR) furnace,
shape than
EBCHR process
Hence,
process
refiningg.
speed and ingot
independent
ratio
superalloy
a Cold-Hearth
to melting is
Beam melting
the evaporation Mitchell'
suggests
of magnesium that
the
rate
evaporation evaporation
rate 10
Herbertson transfer at
an activity
that
in liquid -1 S at
appears
suggested nickel,
that
and 3.6 is
and Calcium
for
nickel
While
this
magnesium
and
Mg-Ni solid
the
liquid
diagram
the
is
known
the
17 .
percent several
In these
As in
is
terms systems
containing
probably
the
liquid solid
of
are
iron
m
mean that
mass transfer important
in
EBCHR refining.
better
known
than
nickel
alloys
are
for
as a best
many
systems,
approximation. in
the
case
of
incomplete, the binary systems Mg-Fe 14,15 . Nickel-magnesium exhibits
phase
and two intermetallic has
an extensive
intermetallic
phases.
and calcium-iron
tentative
-4
from correct.
iron-calcium
no
would
during
when data
for
is
of 1.2 x 10
is
solutions for
far
diagram
than
the
calcium
in
liquid and
miscibility The
iron
is
situation
is
The Ca-Fe
phase
only
is well
0.032
nickel-calcium
complete
in
gap in
diagram 16 , but it
system,
compounds
compounds
systems.
Mg-Fe
nickel-magnesium
intermetalllc
of activity the In
1 as the also
the
magnesium
weight exhibits
solubility
in
the
.
attractions. than
more
those
opposites
solubility
solid 18
is
unity.
Alloys
approach
calcium-nickel
even
that
and
of
-3 for of 10 This
evaporation
of dilute iron 12,13 . Therefore,
a valid it
for
assuming
superalloy
coefficient
and Iron
apply
whereas
phase for
liquid
data
in
phase,
similar
liquid
by Mitchell'
activity
the
essentially
solubility
the
the
by a combination step
Mg-Fe phase
are
complete
in
value
of liquid
in Nickel
and calcium the
by bulk mass -1 -1 of 1.5 x 10 m s
controlled
solutions
may be
While
controlled
constant
many investigators
lacking,
is
at an evaporation rate -1 at 17OO"Cll. x 10e4m s
rate-controlling
The thermodynamic those
rate
coefficient
Hence,
the
Magnesium
magnesium
activity
evaporation
determining
evaporation
evaporation rate constant 10 Herbertson has arrived at this
for
evaporation.
and
the
evaporation step and gives an -1 at 1700°C. On the other hand, m s
one arrives
1700°C
magnesium
the
-7
a Langmuir
coefficient
the
by
of 2.5 x 10
constant
gives It
1700°C.
controlled
claims
and
Using
is
like
one can then
atom attractions
contrast,
intermetallic
confirmed
data
in nickel compounds
are solutions
indicate by Meysson and Rist 19 for
calcium.
410
expect
y
Ca'YMg stronger than
> 1 in iron the
yCa/yMg ought unlike nickel
unlike
atom
to be smaller
atom attraction. and iron-rich
as in
This solutions
20
de Barbadillo on the
solubility
chromium
the
for
based system
the
the
Figure
data
for
instance,
insufficient ternary
3 reproduces
the binary
elements iron
and
data
are
liquid
phase
estimated activity 21 system and data for
Ni-Mg
MQ
d activity .
of magnesium
in
the Fe-Ni-Mg
and Calcium study
alloys
data
may be useful
forgotten
a tentative
system.
alloying
For
alloys.
manages to propose
3:
on these the
nickel
of other While
limited 22 . Ni-Fe-Mg
done alloys
in
influence
solubility.
Fe-Ni-Mg
No experimental nickel-base
the
magnesium
on the
Figure
Magnesium
discusses
magnesium
de Barbadillo
diagram data
of
decreases
available
also
has
elements in
different
of
been
found
in
various
solubility
TABLE I:
deoxidation in
into
Deoxidation
Reaction
the
equilibria
Mg/Ca
account
Ca + 0 = CaO
Mg + 0 * MgO
the
in using
Equilibria log K
equilibria
in
two
I
in solvents
the data
in Iron
Mg and Ca in
Some work has been 23-26 . While these
solutions
deoxidation of
of
literature.
iron-based
establishing
and must be taken
Deoxidation
the
nickel-base cannot
of Tables
I & II.
Alloys
r (“Cl
Ref.
1.8 x 1013 7.9 x 1013
1600
28
1600
27
1.7 x 1o13
1600
23
6.2 x lo5 1.1 x lo6
1600 1600
23 24,25
5.5 x lo5
1600
24,25
K
i
i 7
411
be
TABLE II:
Deoxidation
Equilibria
in Nice1
Alloys
EXPERIMENTAL The
technique
nickel-base
used
alloys
was the
atomic-absorption reference
to
determine novel
the
one of
spectrophotometer.
29.
The
Mg + Sn alloys.
system
activity measuring
vapour
The experimental
was calibrated
The equilibrium
coefficient
constant
using for
pressure
details
both
of
pure
are
Mg in with
an
given
in
magnesium
and
the reaction:
@(is) = h]Ni was determined
as: log K = 2.7
The (kO.2)
Raoultian
activity
x 10
-2
substantially
, with change
as shown in Figure
at 145OOC
coefficient of Mg at 145O'C was found to be 1.2 e Mg = -28 . The addition of Al, Fe and Cr did not 0 these values in the concentration ranges up to 50% Ni,
4.
A no addition 0 20% Fe 0 20% Cr
log ( pMg'
Figure
4:
Comparison between data for alloys containing no major additions and alloys containing 20% Fe or 20% Cr.
412
DISCUSSION
Using
the
data
given
various
process
steps
values.
Since
[MglNi
W,
we are
able
forms 1%I,, , The
for
in
all
observed
expected
VIM
during the
that
depletion
rate
of a 5 tonne
melting
This
data
of Inconel Figure
and indicate
the
practically
with
with
oxygen form
and is
in
present
MgS and
a system as solid
is aprpoximately
an addition
10 ppm
of 150 ppm Mg, and
[MglNi.
the
rates
and
bulk
diffusion
latter
controls the evaporation -5 g cm2 s -1 is estimated for of 1.5 x 10 VIM melt
of Inconel
value
accounts
718,
well
equivalent
for
5.
that
generated 718 melted
These after
above,
by ESR, through
values
ESR all
we can also
the
to a
"Mg-fade"
also the
compare
ingot
well
with
0 o.g 0.8
0.7
Mole Fraction Mg x 1OE-6
Equilibria for: Figure 5: Calculated or ESR slags * 2MgO + [Ti] f 2[Mgl + W.02) Inconel on 40CaF2: 30CaO: 30A1203 and alloy
based 718
the
containing observed
Mg is as MgO or MgS.
1
413
calculate
a slag
1.1
u) 2 c
observed
of Mg in the three
small,
all this
Mg giving
stages.
extremely in
of
and casting.
thermodynamic
MgO, as shown in practice
indicates
losses
the levels
evaporation
5 ppm Mg/min.
Mg contents
is
the
in equilibrium
process
MgO is
Langmuir
conditions of
that
to estimate
the magnesium
A surface
Using
same time
of
with
include
In a VIM melt
of
in
loss
also
superalloy.
coefficients
bulk
must
these
MgO, we can assume that
comparison
the melting
compare
the maximum Mg present
10 wm S, almost
process.
and
product
pure
a typical
we may compute
MgS and MgO at the various
Therefore
A
the
solubility
contained MgO.
at
above
The
loss-rate
of
Mg
from
calculated.
In
an
ingot
conditions,
the
loss
rate
is the
removed ingot
several
of
magnesium
same is
true
of
VAR may
under
which
typical
indicates
also
be
industrial
that
all
[Mg]Ni
of Mg from MgS and MgO as
that
content.
It
retention
of
an
high
the more
that
mechanical
properties.
yet
it
is
is
the
view
of
Mg removal this
with
form the
in of
as
have
note
that
at
a
intermediate-temperature at the residual
levels
likely
any
as
tht
of
the Mg in
sufficiently-low
make
Programme)
during
are grateful the course
for
the
of this
support
may be obtained
of VAR or EB.
of the Teledyne
work. 1
log $pm Mgl
Figie+6;
Reaction Equilibria s] = MgS(s) in Inconel
414
for: 718
this
sulphur
ACKNOWLEDGEMENTS The authors
is
to be noted
ESR, will
ductility
it
permit
content is
The
low sulphur
not It
all
behaviour
a very
MgS will
such
alloy
EB and VAR,
VAR or EB melting. step,
liquid
dissociation
MgS at
but of
of MgS or MgO.
both
way should
dissociation
de-sulphurizing
contents
in
718,
the elimination
at room temperature
for
We also
in Inconel the
10 ppm sulphur
adequate
been observed in
In
the
on
must be through
a VAR alloy
compatible
possible.
magnesium
impact
The MgS carried
processed
than is
but
capacity
appears
(